ASTM

%C

%Mn

%Si

%S

%P

%Al

DC04

St4

CS1

FEP04

SAE 1006

.03 – .06

.18 – .40

.02 max

.02 max

.02 max

.02 max

DC04/DC03

St4/RRSt3

CS1/CS3

FEP04

SAE 1006

ES

.04 – .08

.40 max

.03 max

.02 max

.02 max

.02 max

DC01

St2

CS4

FEP01

SAE 1010

C

.08 – .13

.30 – .40

.03 max

.03 max

.03 max

.03 max

SAE 1018

.14 – .17

.60 – .80

.15 – .25

.02 max

.025 max

.025 max

 

EN 10139 : 1998 Mechanical Properties

Mechanical Properties

Period Delivery

Symbol

Re

Rm

Elongation

Hardness HV

Guaranteed Condition   N/mm2 N/mm2 % min A80  
3 months Annealed A 270-390 28 105 max
Skin passed LC 280 max 270-410 28 115 max
Work hardened C290 200-380 290-430 18 95-125
C340 250 min 340-490 105-155
C390 310 min 390-540 117-172
C440 360 min 440-590 135-185
C490 420 min 490-640 155-200
C590 520 min 590-740 185-225
C690 630 min 690 min 215 min
6 months Annealed A 270-370 34 100 max
Skin passed LC 240 max 270-370 34 110 max
Work hardened C290 210-355 290-390 22 95-117 Temper rolled H1
C340 240 min 340-440 105-130 Temper rolled H2
C390 330 min 390-490 117-155
C440 380 min 440-540 135-172 Temper rolled H3
C490 440 min 490-590 155-185
C590 540 min 590 min 185 min